MP35N

MP35N Material grades and equivalents

MP35N/UNS R30035/ W.Nr 2.4999/ AMS 5844


Introduction:

MP35N is a nickel-cobalt base alloy of the Multiphase alloy system that has a unique combination of properties-ultra high strength, toughness, ductility and outstanding corrosion resistance. The alloy is work-strengthened and aged to obtain strength levels of 260 to 300 ksi(1793-2068 MPa). MP35N alloy resists corrosion in hydrogen sulfide, salt water and other chloride solution, as well as the mineral acids(nitric, hydrochloric, sulfuric).In addition, it has exceptional resistance to crevice and stress corrosion cracking in sea water and other hostile environments.

Chemical composition:

Weight%

Ni

Co

Cr

Mo

Ti

Fe

Si

Mn

P

B

S

C

MP35N

33

Balance

19

9

1

1

0.15

0.15

0.015

0.01

0.01

0.03

37

21

10.5

Max

Max

Max

Max

Max

Max

Max

Max



Mechanical properties:

MP35N Alloy

Ultimate Tensile Strength

0.2% Offset Yield Strength

Elongation in 4D

Reduction of Area

Hardness

Shear
Strength**

Typical Properties
of Solution Treated
(Annealed)

130 ksi(896 MPa)

55 ksi(379 MPa)

65%

75%

90 HRB

—

Typical Properties
of AMS 5844 Product after 4 Hour Age at 1050℉(556℃)*

290 ksi(2000 MPa)

280 ksi(1931 MPa)

10%

45%

51 HRC

—

AMS 5844 Specification Requirements after Aging 4 Hours at 1000-1200℉
(538-648℃)

260 ksi(1795 MPa),min.

230 ksi(1585 MPa),min.

8%,min.

35%,min.

—

150 ksi(1034 Mpa),min.


The above data are longitudinal properties.

*Tensile properties will change depending on product size.

**Not required by AMS 5844, but this is guaranteed shear strength.


Regular shape for all kinds of alloys
Form Specification Supply Form Others
Sheet Thickness:0.40-4.75mm,General Width:1000、1219、1500mm Whole Coil or piece of it Cold Annealed,Surface 2B、2E
Plate Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) Whole Coil or piece of it Single hot rolling,Solid solution annealed state,Surface 1D
Belt Thickness:0.10-3.0mm,Width:50-500mm Whole Coil or Specified size Cold Annealed,Surface 2B、2E
Bar & Rod Rolled barΦ5-45mm,Length≤1500mm Polished Bar(circle、Square) Solution annealing,descaling
Forged barΦ26-245mm,Length≤4000mm
Weld tube Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm Base on your requirement
Seamless Tube Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm Base on your requirement
Wire Outer diameterΦ0.1-13mm Base on your requirement Ni & Ni alloy, Ti & Ti alloy
Forged piece discs,rings,squares,blocks,slabs Base on your requirement Steel, Alloy
Flangs All kinds of Flangs Base on your requirement Steel, Alloy
Welding Material Coil wire Φ0.025mm-1.6mm Base on your requirement Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France.
Straight WireΦ1.6mm-4.0mm
Welding rodΦ1.2mm-4.0mm
Tube Elbow, three links, four links, different diameter size Base on your requirement Ni & Ni alloy, Ti & Ti alloy
Explosive bonded laminate Raw Sheet Thickness≥2mm Base on your requirement Ni & Ni alloy, Ti & Ti alloy